The size of WC grains is of great significance to the friction and wear properties of cemented carbide. It is generally believed that coarse-grained cemented carbide has poorer wear resistance than fine-grained cemented carbide. After the grain refinement of cemented carbide, the size of the hard phase decreases, increasing the surface area of the hard phase grains and the bonding force between the grains, and the binder phase is more evenly distributed around them, which can improve the hardness and wear resistance of the cemented carbide. In this paper, the author conducts friction and wear experiments on cemented carbide to analyze the friction and wear properties under different parameters and the material removal mechanism, providing experimental evidence for the optimization design of high-speed cutting tool materials, reasonable material selection, and the study of high-speed cutting wear mechanisms.

Experiment

Test Materials

Three types of WC-6Co cemented carbide with different grain sizes were selected for the test. The size of the cemented carbide disc was φ55mm×4mm, and the surface was rough ground, finely ground, and polished. The mating material used was Al?O? balls with a diameter of 9.5mm. Both samples were ultrasonically cleaned in acetone for 20 minutes and dried for use. The material properties are shown in Table 1.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 2

Friction and Wear Test

The test was conducted on a UMT-2 multi-functional friction and wear testing machine produced by CETR Corporation in the United States, using a ball-on-disc contact method. The structure of the testing machine is shown in Figure 1. The cemented carbide friction disc was attached to the working table with double-sided tape, and the Al?O? ball was placed in the fixture. The two types of mating materials produced mutual movement and force of action. The friction force generated was detected by the sensor, and the curves of friction force, normal force, and friction coefficient were automatically generated by the related software according to Coulomb’s law.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 3

The test was conducted at room temperature, with normal forces of 10N and 20N respectively, and the linear velocities of the friction pair sliding were 40m/min, 80m/min, 120m/min, and 160m/min. The sliding distance was 500m. After the test, a scanning electron microscope (SEM) was used to observe the wear scar surface morphology of the upper and lower samples, and an X-ray energy dispersive spectrometer (EDS) was used to detect the elemental composition of the worn surfaces. All samples were analyzed for the elemental composition of the friction and wear surfaces under the same conditions.

Results and Analysis

Friction and Wear Performance

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 4

Figure 2 shows the friction coefficient curve of ZH cemented carbide drawn by the testing machine’s accompanying software (load 20N, sliding speed 160m/min). The experiment found that each friction process follows a similar pattern, that is, the initial dynamic friction coefficient undergoes a rapid increase from the initial value during the transition period, and then remains relatively stable, showing a fluctuating characteristic in the stable phase. In the beginning, under the action of the normal load, only local micro-convex bodies on the friction surface are in contact, the adhesive area is small, and the molecular attraction on the contact surface is weak, so the friction coefficient is small; as the friction process progresses, the micro-convex bodies interfere with each other, gradually get worn down, the adhesive area increases, and the molecular attraction also increases, leading to a gradual increase in the friction coefficient. The entire friction process is a continuous process of the contact surface adhering and then being sheared under the action of shear stress. Due to the peeling and breaking of the Co phase on the surface, the wear of the sample surface occurs, and the local adhesion on the surface quickly reaches a dynamic equilibrium, resulting in the friction coefficient of the surface being maintained within a relatively stable range, which is called the stable period.

Most scholars use the average value of the friction coefficient over a period of time (distance) as a characterization parameter of friction behavior. Therefore, this experiment selects the average value during the stable friction phase as the friction coefficient of the cemented carbide under the corresponding parameters. Figure 3 shows the friction coefficients of three types of cemented carbide under different loads and speeds.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 5

It can be seen that with the increase of friction speed and load, the friction coefficient of the cemented carbide generally shows a decreasing trend, and the decrease is most obvious in the transition from relatively low speed (40m/min and 80m/min) to high speed (120m/min and 160m/min). From the perspective of material, the friction coefficient of ZH cemented carbide is smaller than that of the other two materials, and the friction coefficients of ZHX and HG cemented carbides are not significantly different, with the friction coefficient of HG cemented carbide being slightly larger.

Wear Mechanism

After the friction and wear tests, the microstructure of the worn surfaces of each sample was observed using a scanning electron microscope (SEM), and SEM images were taken, along with an analysis of the surface composition. The friction and wear mechanisms of the cemented carbide under different friction parameters are similar, as shown in Figure 4 (sliding speed 160m/min, load 20N).

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 6

In the initial stage of cemented carbide wear, the binder phase Co undergoes plastic deformation, and the surface layer of Co is extruded by the WC grains. Due to the low hardness and good ductility of Co, under certain conditions, a micron-scale friction film can form on the surface, while the harder WC particles gradually protrude from the friction surface, preventing further rapid wear of the surface and allowing the friction process to enter a relatively stable stage. As the binder phase Co continues to be lost, the WC framework of the material is damaged, and the dislocation density within the WC particles significantly increases. When the dislocation density accumulates to a certain extent, microcracks will form on the WC particles, causing the WC particles to begin to pull out from the cemented carbide matrix. The detached WC particles remain in the wear area, transforming into abrasive particles, which, under the action of the load, compress against the matrix, resulting in new plastic deformation and grain damage.

cemented carbide

As can be seen from Figure 4, as the grain size of the cemented carbide decreases, the grain density increases, and the degree of surface wear decreases. The surface of the ZHX cemented carbide shows no obvious shedding of WC particles, while the surface density of HG is very good, with almost no obvious shedding of WC particles. Therefore, for the traditional grain size cemented carbide ZH, the main wear mechanism is abrasive wear caused by the extrusion of the binder phase Co and the shedding of WC grains. As the grain size decreases and the density of the fine-grained cemented carbide increases, the phenomenon of WC grain spalling decreases, Co still wraps around the WC, the microstructure of the material remains intact, and most grains only undergo a certain degree of plastic deformation.

??

The size of WC grains has an important effect on the friction and wear properties of cemented carbide. As the grain size decreases, the friction coefficient slightly increases, and the wear resistance is enhanced.

The friction coefficient of cemented carbide is influenced by speed and load, and it shows a decreasing trend with the increase of speed and load.

The wear mechanism of traditional grain size cemented carbide is mainly characterized by the extrusion of the binder phase Co and the fracture and spalling of the hard phase WC grains; the grain spalling phenomenon of fine-grained cemented carbide is not obvious, and the main wear mechanism is plastic deformation.

?? ???

???? ???? ????. ?? ???? * ? ???? ????

金坛市| 精品国产一区二区三区av-国产精品国产三级国产av播-精品乱人码一区二区三区和四区-成人久久久精品一区二区三区| 曲阳县| 白白嫩嫩国产在线观看-亚洲视频在线观看中文字幕-一区二区三区乱码在线中文老阿姨-亚洲一区av在线免费观看| 徐水县| 泸溪县| 锡林郭勒盟| 高潮喷水亚洲精品视频-中文字幕乱码在线高清完整版-韩国三级永久免费看片-狠狠躁夜夜躁人爽碰人妻视频| 重庆市| 亚洲国产精品一区二区三区色-白嫩肥妇一区二区三区av-久久精品国产亚洲av高清-风韵犹存丰满大屁股熟女国产| 亚洲天堂精品在线观看-久久精品国产亚洲av熟女-国产伦精品二区三区在线观看-美女人妻少妇一区二区三区| 国产成人精品久久一二三区-99久久精品熟女高潮免费-99精品人妻少妇一区二区三区-亚洲中文欧美日韩精品| 洞口县| 亚洲国产精品一区二区三区色-白嫩肥妇一区二区三区av-久久精品国产亚洲av高清-风韵犹存丰满大屁股熟女国产| 武功县| 国产露脸精品国产人妻-国产精品三级一区二区久久久-久久青草亚洲AV无码麻豆-国产蜜臀av在线一区二区三区| 环江| 久久久国产一区二区三区丝袜-中文字幕人妻丝袜成熟乱蜜桃-日本伦理片少妇精油按摩-精品人人妻人人澡人人爽牛牛| 男女猛烈国产无遮挡免费-色噜噜人妻丝袜av影音先-精品国产激情在线成人av-欧美日韩另类丝袜中文| 精品国产一区二区三区av-国产精品国产三级国产av播-精品乱人码一区二区三区和四区-成人久久久精品一区二区三区| 亚洲欧美丝袜清纯另类-丰满人妻熟妇乱又伦精品劲-欧美一级一片内射播放视频-经典有码中文字幕一区二区三区| 久久精品国产96精品亚洲-中文字幕有码视频在线观看-日本黄色激情按摩作爱啪啪视频-欧美激情欧美啪欧美视频| 安福县| 国产艳妇av在线观看果冻传媒-97人妻精品一区二区免费-国产成人三级一区二区在线观看-日韩av大片一区二区三区| 苏尼特右旗| 凤翔县| 亚洲熟妇少妇一区二区三区-污污污十八禁在线观看-国产一区二区三区毛片av-伊人久久综合免费观看完整版| 叙永县| 崇左市| 长宁区| 遵义县| 黄色加黑色播放器在线观看-国产又粗又猛又爽又黄久久精品-手机在线免费观看岛国av-婷婷丁香开心综合人妻系列| 平利县| 通海县| 视频| 金昌市| 熟女人妻一区二区在线观看-国产欧美激情视频在线观看-最新亚洲av网址在线观看-毛片在线观看免费日韩| 国产亚洲性色av大片久久香蕉-91亚洲精品国产自在现线-国产在线精品免费播放-日韩中文字幕国产精品| 岛国精品一区二区三区不卡-精品一区二区三区不卡少妇av-中文字幕人妻丝袜乱一区二区三区-久久精品国产亚洲av成人乳| 中文字幕理伦午夜福利片-日韩精品高清免费视频-被夫上司强暴的人妻中文字幕-国产一区二区三区精品av| 阳原县|