The size of WC grains is of great significance to the friction and wear properties of cemented carbide. It is generally believed that coarse-grained cemented carbide has poorer wear resistance than fine-grained cemented carbide. After the grain refinement of cemented carbide, the size of the hard phase decreases, increasing the surface area of the hard phase grains and the bonding force between the grains, and the binder phase is more evenly distributed around them, which can improve the hardness and wear resistance of the cemented carbide. In this paper, the author conducts friction and wear experiments on cemented carbide to analyze the friction and wear properties under different parameters and the material removal mechanism, providing experimental evidence for the optimization design of high-speed cutting tool materials, reasonable material selection, and the study of high-speed cutting wear mechanisms.

Experiment

Test Materials

Three types of WC-6Co cemented carbide with different grain sizes were selected for the test. The size of the cemented carbide disc was φ55mm×4mm, and the surface was rough ground, finely ground, and polished. The mating material used was Al?O? balls with a diameter of 9.5mm. Both samples were ultrasonically cleaned in acetone for 20 minutes and dried for use. The material properties are shown in Table 1.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 2

Friction and Wear Test

The test was conducted on a UMT-2 multi-functional friction and wear testing machine produced by CETR Corporation in the United States, using a ball-on-disc contact method. The structure of the testing machine is shown in Figure 1. The cemented carbide friction disc was attached to the working table with double-sided tape, and the Al?O? ball was placed in the fixture. The two types of mating materials produced mutual movement and force of action. The friction force generated was detected by the sensor, and the curves of friction force, normal force, and friction coefficient were automatically generated by the related software according to Coulomb’s law.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 3

The test was conducted at room temperature, with normal forces of 10N and 20N respectively, and the linear velocities of the friction pair sliding were 40m/min, 80m/min, 120m/min, and 160m/min. The sliding distance was 500m. After the test, a scanning electron microscope (SEM) was used to observe the wear scar surface morphology of the upper and lower samples, and an X-ray energy dispersive spectrometer (EDS) was used to detect the elemental composition of the worn surfaces. All samples were analyzed for the elemental composition of the friction and wear surfaces under the same conditions.

Results and Analysis

Friction and Wear Performance

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 4

Figure 2 shows the friction coefficient curve of ZH cemented carbide drawn by the testing machine’s accompanying software (load 20N, sliding speed 160m/min). The experiment found that each friction process follows a similar pattern, that is, the initial dynamic friction coefficient undergoes a rapid increase from the initial value during the transition period, and then remains relatively stable, showing a fluctuating characteristic in the stable phase. In the beginning, under the action of the normal load, only local micro-convex bodies on the friction surface are in contact, the adhesive area is small, and the molecular attraction on the contact surface is weak, so the friction coefficient is small; as the friction process progresses, the micro-convex bodies interfere with each other, gradually get worn down, the adhesive area increases, and the molecular attraction also increases, leading to a gradual increase in the friction coefficient. The entire friction process is a continuous process of the contact surface adhering and then being sheared under the action of shear stress. Due to the peeling and breaking of the Co phase on the surface, the wear of the sample surface occurs, and the local adhesion on the surface quickly reaches a dynamic equilibrium, resulting in the friction coefficient of the surface being maintained within a relatively stable range, which is called the stable period.

Most scholars use the average value of the friction coefficient over a period of time (distance) as a characterization parameter of friction behavior. Therefore, this experiment selects the average value during the stable friction phase as the friction coefficient of the cemented carbide under the corresponding parameters. Figure 3 shows the friction coefficients of three types of cemented carbide under different loads and speeds.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 5

It can be seen that with the increase of friction speed and load, the friction coefficient of the cemented carbide generally shows a decreasing trend, and the decrease is most obvious in the transition from relatively low speed (40m/min and 80m/min) to high speed (120m/min and 160m/min). From the perspective of material, the friction coefficient of ZH cemented carbide is smaller than that of the other two materials, and the friction coefficients of ZHX and HG cemented carbides are not significantly different, with the friction coefficient of HG cemented carbide being slightly larger.

Wear Mechanism

After the friction and wear tests, the microstructure of the worn surfaces of each sample was observed using a scanning electron microscope (SEM), and SEM images were taken, along with an analysis of the surface composition. The friction and wear mechanisms of the cemented carbide under different friction parameters are similar, as shown in Figure 4 (sliding speed 160m/min, load 20N).

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 6

In the initial stage of cemented carbide wear, the binder phase Co undergoes plastic deformation, and the surface layer of Co is extruded by the WC grains. Due to the low hardness and good ductility of Co, under certain conditions, a micron-scale friction film can form on the surface, while the harder WC particles gradually protrude from the friction surface, preventing further rapid wear of the surface and allowing the friction process to enter a relatively stable stage. As the binder phase Co continues to be lost, the WC framework of the material is damaged, and the dislocation density within the WC particles significantly increases. When the dislocation density accumulates to a certain extent, microcracks will form on the WC particles, causing the WC particles to begin to pull out from the cemented carbide matrix. The detached WC particles remain in the wear area, transforming into abrasive particles, which, under the action of the load, compress against the matrix, resulting in new plastic deformation and grain damage.

cemented carbide

As can be seen from Figure 4, as the grain size of the cemented carbide decreases, the grain density increases, and the degree of surface wear decreases. The surface of the ZHX cemented carbide shows no obvious shedding of WC particles, while the surface density of HG is very good, with almost no obvious shedding of WC particles. Therefore, for the traditional grain size cemented carbide ZH, the main wear mechanism is abrasive wear caused by the extrusion of the binder phase Co and the shedding of WC grains. As the grain size decreases and the density of the fine-grained cemented carbide increases, the phenomenon of WC grain spalling decreases, Co still wraps around the WC, the microstructure of the material remains intact, and most grains only undergo a certain degree of plastic deformation.

Conclus?o

The size of WC grains has an important effect on the friction and wear properties of cemented carbide. As the grain size decreases, the friction coefficient slightly increases, and the wear resistance is enhanced.

The friction coefficient of cemented carbide is influenced by speed and load, and it shows a decreasing trend with the increase of speed and load.

The wear mechanism of traditional grain size cemented carbide is mainly characterized by the extrusion of the binder phase Co and the fracture and spalling of the hard phase WC grains; the grain spalling phenomenon of fine-grained cemented carbide is not obvious, and the main wear mechanism is plastic deformation.

Deixe uma resposta

O seu endere?o de e-mail n?o será publicado. Campos obrigatórios s?o marcados com *

久久精品人妻一区二区三区不卡-日韩亚洲熟女少妇一区二区三区-在线观看国产超级av-成年人视频日本大香蕉久久| 97精品人妻一区二区三区麻豆-亚洲最大av在线观看网址-欧美日韩精品一区二区三区不卡-亚洲熟伦熟女新五十路熟女| 97精品人妻一区二区三区麻豆-亚洲最大av在线观看网址-欧美日韩精品一区二区三区不卡-亚洲熟伦熟女新五十路熟女| 门头沟区| 高潮喷水亚洲精品视频-中文字幕乱码在线高清完整版-韩国三级永久免费看片-狠狠躁夜夜躁人爽碰人妻视频| 白白嫩嫩国产在线观看-亚洲视频在线观看中文字幕-一区二区三区乱码在线中文老阿姨-亚洲一区av在线免费观看| 山西省| 新蔡县| 乐清市| 丰满少妇被粗大猛烈进人高清视频-中文字幕亚洲精品乱码在线看-91麻豆精品成人免费视频-好爽好硬好深好大好紧视频| 灵山县| 东山县| 国产精品剧情一区二区三区av-白丝美女被狂操视频在线观看-午夜精品一区二区三区成人-亚洲熟妇av一区二区三区不卡| 亚洲精品国产av一区二区三区-国家一级—片内射视频播放免费-欧美日本高清在线不卡视频-国产人妻熟女开裆丝袜| 沿河| 德昌县| 天堂最新在线资源欧美-97超碰人人模人人爽人人爱-免费久久99精品国产婷婷六月-看香蕉视频一直看一直爽| 国产伊人成人在线视频-亚洲av日韩激情在线观看-国产资源精品中文字幕-久久久999精品免费视频| 性感校花被我无套内射在线观看-国产亚洲中文久久网久久综合-男j进女屁股视频在线观看-欧美成人一区二区三区在线观看| 无为县| 甘孜县| 激情五月色播天美果冻传媒-亚洲国产av一卡二卡-中文乱码精品一区二区三区人妻-日韩av中出一区二区三区| 团风县| 隆回县| 中文字幕最新有码在线-91亚洲国产一区二区三区-国内精品伊人久久久av高清-国产成人精品午夜在线播放| 武邑县| 佛坪县| 济宁市| 白白嫩嫩国产在线观看-亚洲视频在线观看中文字幕-一区二区三区乱码在线中文老阿姨-亚洲一区av在线免费观看| 郯城县| 国产欧美日韩中文久久-一区二区三区少妇熟女高潮-99久久婷婷国产综合亚洲-国产露出精品一区二区三区91| 黄大仙区| 桑日县| 内黄县| 久久精品国产亚洲av试看-风韵饥渴的中年富婆偷人视频-99久久久精品国产美女-日本高清av一区二区三区| 国产精品十八禁亚洲黄污免费观看-国产成人久久久精品二区三-国产美女都是黄色的视频-国产成人精品一区二区三区| 达孜县| 色哟哟精品一区二区三区四区-精品人妻一区二区三区蜜桃九-婷婷久久亚洲中文字幕-国产久久热这里只有精品| 国产老熟女高潮精品视频-精品国产亚洲av在线观看-78国产伦精品一区二区三区-久久91精品国产91久久麻豆| 咸宁市| 安溪县|